Acid
video
Acid

Acid Potassium Chloride Zinc Electroplating Softener

Potassium chloride type weakly acidic galvanizing electrolyte Potassium chloride type weakly acidic zinc plating electrolyte additives factory Zinc plating brightener Cost saving solution provider Zinc plating bath brightening agent Zinc plating technological process expert Cost saving solution provider Zinc electroplating acid chemical solution additives manufacturer Here are the parts after zinc plated from our client’s workshop Chemical bath brightening agent Process design expert team Professional technical support Production process optimization and improvement

Description

It is characterized by simple electrolyte composition, stable electrolyte, fine coating, bright, high current efficiency, wide operating temperature range (5 ~ 60℃), simple wastewater treatment. The chemical dissolution of the anode in the electrolytic cell leads to the increase of the concentration of main salt ions in the electrolyte.

 

Common failures and processing method

Problem Description

Probable cause

Solutions

 

 

 

Poor brightness

Lack of brightener

Lack of softener

Organic

impurity pollution

Brightener supplement

Softener supplement

Activated

carbon filtration

 

Poor coverage

No coating in hole and concave

 

Lack of brightener

Lack of softener

Low potassium chloride

The bath temperature

becomes higher

Aluminum

impurity pollution

Brightener supplement

Softener supplement

Potassium

chloride supplement

Lowering temperature

Treat with zinc powder

 

The bright range is narrow and the coating is easy to burn

 

The PH value of the bath increases

Lack of zinc

Lack of boric acid

Lack of softener

Adjust PH value with dilute hydrochloric acid

Zinc

chloride supplement

Boric acid supplement

Softener supplement

 

The coating has white mist

 

Effect of

organic impurities

Poor cleaning after plating

Activated

carbon filtration

Change the

cleaning water

 

The coating blackening after acid dipping

Iron impurity

Copper impurity

Hydrogen peroxide treatment and filtration

Treat with zinc powder

 

Roller holes appear

in the coating

 

Lack of softener

Iron impurity

Excessive current

Lower zinc

Over loading of work

 

Softener supplement

Hydrogen peroxide treatment and filtration

Lower total current

Zinc

chloride supplement

Reduced loading

 

Hot Tags: acid potassium chloride zinc electroplating softener, China acid potassium chloride zinc electroplating softener manufacturers, suppliers, factory

(0/10)